HEATS 发表于 2010-9-12 10:21:29

高温合金的切削加工中铣削高温合金切削用量举例-端铣刀铣削

<TABLE cellSpacing=0 cellPadding=0 width="100%" border=1>
<TBODY>
<TR>
<TD width="100%" colSpan=6>
<DIV align=center>端铣刀铣削</DIV></TD></TR>
<TR>
<TD width="9%">
<DIV align=center>工件材料</DIV></TD>
<TD width="15%">
<DIV align=center>刀具牌号</DIV></TD>
<TD width="25%">
<DIV align=center>轴向切削深度αp(mm)</DIV></TD>
<TD width="20%">
<DIV align=center>每转进给量αf(mm)</DIV></TD>
<TD width="18%">
<DIV align=center>切削速度v(m/min)</DIV></TD>
<TD width="11%">
<DIV align=center><SUB>切削液</SUB></DIV></TD></TR>
<TR>
<TD>
<DIV align=center>GH37</DIV></TD>
<TD>
<DIV align=center>W12Cr4V4Mo</DIV></TD>
<TD>
<DIV align=center>1~3</DIV></TD>
<TD>
<DIV align=center>0.1~0.5</DIV></TD>
<TD>
<DIV align=center>9~15</DIV></TD>
<TD>
<DIV align=center>防锈冷却液①</DIV></TD></TR>
<TR>
<TD>
<DIV align=center>GH37</DIV></TD>
<TD>
<DIV align=center>W2Mo9Cr4VCo8</DIV></TD>
<TD>
<DIV align=center>1~3</DIV></TD>
<TD>
<DIV align=center>0.1~0.5</DIV></TD>
<TD>
<DIV align=center>9~15</DIV></TD>
<TD>
<DIV align=center>防锈冷却液①</DIV></TD></TR>
<TR>
<TD>
<DIV align=center>GH37</DIV></TD>
<TD>
<DIV align=center>W18Cr4V</DIV></TD>
<TD>
<DIV align=center>1~3</DIV></TD>
<TD>
<DIV align=center>0.1~0.5</DIV></TD>
<TD>
<DIV align=center>9~15</DIV></TD>
<TD>
<DIV align=center>防锈冷却液①</DIV></TD></TR>
<TR>
<TD>
<DIV align=center>GH36</DIV></TD>
<TD>
<DIV align=center>W18Cr4V</DIV></TD>
<TD>
<DIV align=center>1~3</DIV></TD>
<TD>
<DIV align=center>0.2~0.25</DIV></TD>
<TD>
<DIV align=center>20~25</DIV></TD>
<TD>
<DIV align=center>防锈冷却液</DIV></TD></TR>
<TR>
<TD>
<DIV align=center>GH49</DIV></TD>
<TD>
<DIV align=center>W2Mo9Cr4VCo8</DIV></TD>
<TD>
<DIV align=center>1~3</DIV></TD>
<TD>
<DIV align=center>0.04~0.15</DIV></TD>
<TD>
<DIV align=center>5~8</DIV></TD>
<TD>
<DIV align=center>防锈冷却液</DIV></TD></TR>
<TR>
<TD>
<DIV align=center>GH49</DIV></TD>
<TD>
<DIV align=center>W6Mo5Cr4V2A1</DIV></TD>
<TD>
<DIV align=center>1~3</DIV></TD>
<TD>
<DIV align=center>0.04~0.15</DIV></TD>
<TD>
<DIV align=center>5~8</DIV></TD>
<TD>
<DIV align=center>防锈冷却液</DIV></TD></TR>
<TR>
<TD>
<DIV align=center>GH49</DIV></TD>
<TD>
<DIV align=center>W18Cr4V</DIV></TD>
<TD>
<DIV align=center>1~3</DIV></TD>
<TD>
<DIV align=center>0.04~0.15</DIV></TD>
<TD>
<DIV align=center>5~8</DIV></TD>
<TD>
<DIV align=center>防锈冷却液</DIV></TD></TR>
<TR>
<TD>
<DIV align=center>GH132</DIV></TD>
<TD>
<DIV align=center>W2Mo9Cr4VCo8</DIV></TD>
<TD>
<DIV align=center>1~4~8</DIV></TD>
<TD>
<DIV align=center>0.13~0.2~0.25</DIV></TD>
<TD>
<DIV align=center>18~9~5</DIV></TD>
<TD>
<DIV align=center>防锈冷却液</DIV></TD></TR>
<TR>
<TD>
<DIV align=center>GH136</DIV></TD>
<TD>
<DIV align=center>W2Mo9Cr4VCo8</DIV></TD>
<TD>
<DIV align=center>1~4~8</DIV></TD>
<TD>
<DIV align=center>0.13~0.2~0.25</DIV></TD>
<TD>
<DIV align=center>18~9~5</DIV></TD>
<TD>
<DIV align=center>防锈冷却液</DIV></TD></TR>
<TR>
<TD>
<DIV align=center>K1</DIV></TD>
<TD>
<DIV align=center>W2Mo9Cr4VCo8</DIV></TD>
<TD>
<DIV align=center>0.5~0.55</DIV></TD>
<TD>
<DIV align=center>0.06~0.1</DIV></TD>
<TD>
<DIV align=center>5~3</DIV></TD>
<TD>
<DIV align=center>防锈冷却液</DIV></TD></TR>
<TR>
<TD>
<DIV align=center>k17</DIV></TD>
<TD>
<DIV align=center>W2Mo9Cr4VCo8</DIV></TD>
<TD>
<DIV align=center>1.5~5.5</DIV></TD>
<TD>
<DIV align=center>0.06~0.1</DIV></TD>
<TD>
<DIV align=center>5~3</DIV></TD>
<TD>
<DIV align=center>防锈冷却液</DIV></TD></TR></TBODY></TABLE>
<DIV>注:<BR>① 防锈冷却液成分为三乙醇胺、癸二酸、亚硝酸钠、水<BR>②电解冷却液成分为硼酸、甘油、癸二酸钠、水</DIV>
               